Integrity UltraFibers are 13mm (1/2 inch) alkali-resistant (AR) glass fibers for GFRC, mortar, stucco, parging and concrete. This page explains how much to use and how to mix them for each type of mix.
What UltraFibers Are
Ordinary fiberglass is E-glass, which the high alkalinity of cement attacks over time. UltraFibers contain zirconia that meets ASTM C1666 and EN 15422, so they stay strong inside cement-based mixes.
| Property | UltraFibers | Conventional AR glass |
|---|---|---|
| Filament diameter | 14 microns | 18 microns |
| Bundle weight (tex) | 82 | 135 |
| Filaments per bundle | 200 | 200 |
| Fibers per pound | About 65% more | Baseline |
| Length | 13mm (1/2 inch) | Usually 19mm (3/4 inch) |
UltraFibers are integral fibers: each bundle of 200 filaments is designed to stay together in the mix rather than break apart into single strands. A protective sizing keeps the bundles from shredding into fluff while mixing, so they flow smoothly and show less at the surface than conventional AR glass.
Available in 1 lb and 20 kg (44 lb) bags.
Choose Your Mix
How much fiber to use depends on what’s in the mix. Sand-only mixes can take much more fiber than mixes with gravel.
| Mix | What fibers do | Dose | Per 1 lb bag of UltraFibers |
|---|---|---|---|
| GFRC (such as Integrity PowerBlend) | Primary reinforcement in place of steel | 1.9% of total batch weight | One 45 lb bag of PowerBlend |
| Mortar, stucco, parging, sand mix | Tougher, more crack-resistant mix | About 1% to 1.5% | Up to one 60 to 80 lb bag |
| Aggregate-based concrete (such as 5000 psi bagged mix) | Shrinkage crack control only | 4 to 8 lb per cubic yard | 8 to 10 bags of 60 to 80 lb mix |
Whatever the mix, add the fibers last and mix at slow speed just until they’re evenly dispersed. Overmixing breaks fiber bundles apart.
Percentages are of total batch weight: everything in the mixer, including water, polymer and the fibers themselves.
GFRC: Dosing and Mixing
Use 1.9% UltraFibers by total batch weight. With Integrity PowerBlend, that’s one 1 lb bag of UltraFibers per 45 lb bag of PowerBlend.
In properly made GFRC, AR glass fibers replace steel as the main reinforcement. That depends on the right fiber dose, a thorough mix and careful placement.
Calculating Fibers for Other GFRC Mixes
Fiber load is a share of everything in the batch, including water, polymer and the fibers. To find the fiber weight, weigh or total every other ingredient first:
Fiber weight = weight of all other ingredients x 1.9 / 98.1
Example: a backer batch of sand, cement, pozzolan, polymer and water totaling 79.5 lb needs 79.5 x 1.9 / 98.1 = 1.54 lb of UltraFibers, for an 81.0 lb batch.
For ready-made batch sizes, see the GFRC mix recipes.
Mixing
- Use a handheld paddle mixer, such as a Collomix Xo6 or Xo55. Barrel and tumble mixers can’t put enough energy into a GFRC mix.
- Add PowerBlend to the water in stages: about a third, then half of what’s left, then the rest. Blend until each portion wets out.
- Scrape the bucket and paddle, then mix on medium to high speed for at least 2 full minutes.
- Drop to slow speed. Add the fibers gradually and mix only until they’re fully wetted and dispersed. Never mix fibers on high speed.
Direct Casting
- Chill the mix to 55 to 60°F (13 to 16°C), for example by using ice as part of the mix water. Let the ice melt fully before adding fibers.
- For a pourable consistency, add a little extra UltraFlow.
- Once the fibers are mixed in, let the mix rest undisturbed for 10 to 15 minutes.
- Pour slowly into the mold. Don’t remix after resting.
For large or heavily loaded pieces, pour in several thin lifts rather than one thick pour. More of the fibers lie flat that way, which makes a stronger piece. Here’s why.
For the full process, see CCI’s Integrity PowerBlend page.
Mortar, Stucco and Parging: Dosing and Mixing
Use one 1 lb bag of UltraFibers per 60 to 80 lb bag of mortar, stucco or sand mix. That’s about 1% to 1.5% of total batch weight once water is added.
Mortar, stucco and sand mix contain sand but no gravel, so they can take more fiber than aggregate-based concrete. Fibers spread through the mix and help it resist cracking as it dries, which matters most in thin coats like parging and stucco.
Don’t add UltraFibers to stucco or mortar mixes that already contain fibers. Many bagged “fiber-reinforced” stuccos are made to be used as is.
You may not be able to add an entire 1 lb bag of UltraFibers to one bag of mortar or stucco mix without affecting workability.
- Mix the mortar and water to working consistency first.
- Add a small amount of fibers gradually at slow speed, by hand, with a drill paddle on low speed, or in a mortar mixer.
- Mix just until the fibers are evenly dispersed and the mix retains a workable consistency. Avoid overmixing.
- Keep track of how much fiber you added per bag of mix, since you may not be able to add the full 1 lb of fibers without affecting workability. For example, if you were able to add only 0.5 lb of fibers to 1 bag of mix, add the same amount to the next bag of mix.
Aggregate-Based Concrete: Dosing and Mixing
Use 4 to 8 lb of UltraFibers per cubic yard of concrete. In bagged mix, that’s about 1.5 to 2 oz per 60 to 80 lb bag, so one 1 lb bag treats 8 to 10 bags.
Gravel-based concrete, such as 5000 psi bagged mix, can take far less fiber than GFRC. The coarse aggregate limits how much fiber fits, and more fiber makes the mix stiffer and harder to place.
- Mix the concrete and water first.
- Add the fibers and mix just until they’re evenly dispersed.
- Mix designs vary by brand, so try a small test batch first to check how the fibers affect flow.
A kitchen scale is the easiest way to measure fibers for a single bag of mix.
What Fibers Won’t Do in Regular Concrete
- They control shrinkage cracking only. They are not structural reinforcement.
- They don’t replace rebar.
- Adding fibers to regular concrete doesn’t make it GFRC. GFRC’s strength comes from a much higher fiber load, polymer and a properly designed mix all working together.
Questions
Other fibers say 1 lb per cubic yard. Why is your dose higher?
That dose was developed for dispersible fibers, which break apart into single filaments in the mix. UltraFibers are integral bundles that stay together, so each pound contains fewer separate fibers and you need more weight to get the same coverage. For perspective, 1 lb per cubic yard is about 0.025% of the batch.
What’s the difference between E-glass and AR glass?
E-glass is ordinary fiberglass. Cement is highly alkaline, and over time it weakens E-glass fibers. AR glass contains zirconia, which resists that attack. UltraFibers meet ASTM C1666 and EN 15422 for alkali-resistant glass fiber.
Will the fibers show at the surface?
UltraFibers’ finer filaments and shorter 13mm length show less than conventional AR glass. Any glass fiber can still show if it ends up at the surface, especially after grinding or polishing.
Can fibers replace rebar?
Only in properly made GFRC, where AR glass fibers are the primary reinforcement. In mortar, stucco and regular concrete, fibers control cracking but don’t replace rebar or other structural steel.
Is this fiber mesh?
No. UltraFibers are loose chopped fibers that mix into the concrete, not a mesh sheet or fabric.